Magnetic Characteristics
Former Standard
|
|
Remanence |
Coercivity |
Max.
Energy product |
|||
|
Material Code |
Br |
Hcb |
(BH)max |
|||
|
T |
Gs |
kA/m |
Oe |
kJ/M3 |
MGOe |
|
|
Y10T |
≥0.20 |
≥2000 |
128
–
160 |
1600
–
2000 |
6.4
–9.6 |
0.8
–
1.2 |
|
Y20 |
0.32
–
0.38 |
3200
–
3800 |
128
–
192 |
1600
–
2400 |
18.3
–
21.5 |
2.3
–
2.7 |
|
Y25 |
0.35
–
0.39 |
3500
–
3900 |
152
–
208 |
1900
–
2600 |
22.3
–
25.5 |
2.8
–
3.2 |
|
Y30 |
0.38
–
0.42 |
3800
- 4200 |
160
- 216 |
2000
- 2700 |
26.3
–
29.5 |
3.3
–
3.7 |
|
Y35 |
0.40
–
0.44 |
4000
- 4400 |
176
- 224 |
2200
-2800 |
30.3
–
33.4 |
3.8
–
4.2 |
|
Y20H |
≥0.34 |
≥3400 |
248
- 264 |
3100
- 3300 |
≥21.5 |
≥2.7 |
|
Y25BH |
0.36
–
0.39 |
3600
- 3900 |
224
- 240 |
2800
- 3000 |
23.9
–27.1 |
3.0
–
3.4 |
|
Y30BH |
0.38
–
0.40 |
3800
- 4000 |
224
- 240 |
2800
- 3000 |
27.1
–
30.3 |
3.4
–
3.8 |
|
|
Remanence |
Coercivity |
Intrinsic |
Max.Energy Product |
|
Material |
Br |
Hcb |
Hcj |
(BH)max |
|
Y8T |
200-235 |
125-160 |
210-280 |
6.5-9.5 |
|
Y20 |
320-380 |
135-190 |
140-195 |
18.0-22.0 |
|
Y22H |
310-360 |
220-250 |
280-320 |
20.0-25.4 |
|
Y23 |
320-370 |
170-190 |
190-230 |
20.0-25.4 |
|
Y25 |
360-400 |
135-170 |
140-200 |
22.5-28.0 |
|
Y26H |
360-390 |
220-25 |
225-255 |
23.0-28.0 |
|
Y27H |
370-400 |
205-250 |
210-255 |
25.0-29.5 |
|
Y28 |
370-400 |
175-210 |
180-220 |
26.0-30.0 |
|
Y30H-1 |
380-400 |
230-275 |
235-290 |
27.0-32.0 |
|
Y30H-2 |
395-415 |
275-300 |
310-335 |
28.5-32.5 |
|
Y32 |
400-420 |
160-190 |
165-195 |
30.0-33.5 |
|
Y33 |
410-430 |
220-250 |
225-255 |
31.5-35.0 |
|
Parameters |
Mark |
Unit
|
Values |
Remark |
|
Recoil
Permeability |
Цrec |
Gs/Oe |
1.05-1.3 |
|
|
Curie
Temperature |
Tc |
℃ |
≥450 |
|
|
Temp.
Coefficient of Magnetic Induction |
a(Br) |
℃-1 |
-0.2% |
0-100℃ |
|
Temp.Coefficient
of Inturensic Coerrice force |
a(Hcj) |
℃-1 |
-0.2-0.5% |
0-100℃ |
|
Density |
d
|
g/cm3 |
4.6-5.0 |
|
|
Specific
Resistance |
? |
Ω.cm |
≥106 |
|
|
Coefficient of Thermal Expansion |
|
℃ |
7-15×10-6 |
|
| Hardness | HV | ------ | 480--580 |